Type V Standard Grout
The characteristics itemized below are for a
water/cement ratio of 0.8/1 by weight. Those items with an * can be adjusted as
required by the application.
|
|
Property |
Standards
and Conditions |
Results |
|
Dry |
Dispersant |
0.85%
by weight of dry grout |
|
|
|
Color |
Visual |
Cement gray |
|
|
Particle
Size |
SediGraph
5100 |
90%<8 microns, average 4 microns |
|
|
Surface
Area |
ASTM
C-204 (Blaine Fineness) |
15,110 cm²/gram |
|
|
Dry
Loose Unit Weight |
|
0.497 grams/cc |
|
|
Dry
Density (Specific Gravity) |
ASTM
C-188 |
2.70 grams/cm³ |
|
|
Dry
Weight/Wet Volume |
|
1.01 kg/liter |
|
|
|
|
|
|
Wet |
Water/Grout |
0.8/1 by weight of dry grout * |
|
|
|
Wet
Density (Specific Gravity) |
API
RP 13B-1 (Barold Mud Balance) |
1.56 grams/cc * |
|
|
Initial
Viscosity |
API
RP 13B-1 (Marsh Cone) |
37 seconds * |
|
|
Internal
Cohesion |
Lombardi
Plate |
1.22 Pascals * |
|
|
Initial
Gelation |
Wally
Baker Shear Value |
3.7 hours * |
|
|
Final
Gelation |
Wally
Baker Shear Value |
4.6 hours * |
|
|
Initial
Vicat Needle Set |
ASTM
C-191 (Vicat Needle) |
9.33 hours * |
|
|
Final
Vicat Needle Set |
ASTM
C-191 (Vicat Needle) |
9.83 hours * |
|
|
Period
of Workability |
|
3.6 hours * |
|
|
Shrinkage |
ASTM
C-490, C-596, C-157 |
-0.0260% |
|
|
Bleeding |
ASTM
C-940 |
0.50% |
|
|
Hydrational
Heat |
Adiabatic
Chamber |
31º C |
|
|
Pressure
Filtration |
API
Filter Press |
0.0678 minutes - 1/2 |
|
|
Permeability |
Custom
Equipment at Atomic Energy of Canada |
1x10-16 cm/second |
|
|
Sulfate
Resistant |
Type
V Sulfate Resistant Cement |
Resistant to sulfate attack |
Note: A high shear, so called
"Colloidal" mixer such as the "COLCRETE"
**, should be used for any microfine or
ultrafine cementitious grout.
Contact us at (800)767-4701
or (208)766-4777 or email us at salesmgr@usgrout.com
US Grout
Home
About the Company
Product Applications Mixing
Instructions
**For more information about the
"COLCRETE" colloidal mixer click here and
follow the link to "The Development of Colloidal Mixer Based CRF
System"